Manufacturing Process, Microstructure, and Properties of Small-Diameter S31254 Super Austenitic Stainless Steel Welded Pipes
Abstract: Small-diameter S31254 super-austenitic stainless steel straight-seam welded pipes (Φ32 mm × 1.2 mm) were manufactured using direct-current tungsten inert gas (DC TIG) welding. Their mechanical properties, microstructure, and corrosion resistance were investigated. The results are summarized as follows:
Microstructure: The base metal, weld zone, and heat-affected zone (HAZ) all exhibited an austenitic microstructure. The weld zone was characterized by columnar dendritic grains.
Mechanical properties: The welded pipes achieved a tensile strength of ≥804 MPa, a yield strength of ≥467 MPa, and an elongation of ≥45.8%.
Hardness: The hardness values of the base metal, weld zone, and HAZ were all ≤95.2 HRB.
Process performance: No cracks were observed in the specimens after process performance testing.
Corrosion resistance and nondestructive testing: The welded pipes met all applicable standard requirements for intergranular corrosion, pitting corrosion, and nondestructive testing.
These results demonstrate the reliability of the manufacturing process and the good overall performance of the welded pipes, supporting their suitability for mass production. This study provides a technical reference for manufacturing similar small-diameter super-austenitic stainless steel welded pipes.
S31254 is a nickel–chromium super-austenitic stainless steel characterized by a low carbon content and high contents of molybdenum (Mo), chromium (Cr), nickel (Ni), and nitrogen (N). Its total alloying element content approaches 50%. Chromium and molybdenum promote the formation of a protective passive film on the steel surface, imparting excellent resistance to intergranular corrosion, pitting corrosion, and stress corrosion cracking. Its pitting resistance equivalent number (PREN) is ≥40. Owing to its excellent mechanical properties and weldability, S31254 stainless steel is widely used in pulp and paper production, marine engineering, and the petrochemical industry. However, its high Cr, Ni, and Mo contents also increase its susceptibility to hot cracking during welding. In addition, welding may result in the loss or segregation of alloying elements, potentially compromising the corrosion resistance and mechanical properties of welded joints. Consequently, the welding of S31254 super-austenitic stainless steel has attracted considerable research interest.
Tong Chaogang et al. investigated gas tungsten arc welding (GTAW) with filler wire for 3.68 mm-thick S31254 super-austenitic stainless steel welded pipes intended for a natural gas processing project. Their findings indicated that the welding process should use the lowest possible heat input. The optimal welding parameters included a filler-wire angle of 10°–15° relative to the pipe tangent and a welding-torch angle of 75°–80° relative to the filler wire. These parameters resulted in the best combination of initial pass rate and weld quality. Wenyan Ding et al. investigated the processability and microstructural evolution of high-molybdenum super-austenitic stainless steel pipes during manufacturing. They reported that, for S31254 pipes produced by hot extrusion followed by three-pass cold rolling, high-temperature heat treatment can eliminate detrimental phases, such as the σ phase, formed during earlier processing. Specifically, holding the pipes at 1,150–1,180 °C for 5–10 min, followed by rapid cooling at a rate exceeding 350 °C/min, enables mass-produced S31254 super-austenitic stainless steel seamless pipes to meet the specified requirements for mechanical properties, microstructure, and corrosion resistance.
Although considerable research has been conducted on the manufacturing processes, microstructures, and properties of large-diameter, thick-walled S31254 super-austenitic stainless steel welded and seamless pipes, relatively few studies have focused on the fabrication of small-diameter S31254 welded pipes using direct-current gas tungsten arc welding (DC-GTAW) or on the resulting microstructures and properties. In this study, a manufacturing process was developed for S31254 welded pipes with dimensions of Φ32 mm × 1.2 mm. Their mechanical properties, macroscopic weld appearance, weld microstructure, and corrosion resistance were investigated. The aim was to provide a technical reference for the mass production of small-diameter S31254 welded pipes.
The material used in this study was a cold-rolled and annealed S31254 super-austenitic stainless steel strip measuring 98.7 mm × 1.2 mm. The material complied with ASTM A240/A240M-2023, Standard Specification for Chromium and Chromium-Nickel Stainless Steel Plate, Sheet, and Strip for Pressure Vessels and for General Applications. Its chemical composition is presented in Table 1, and its mechanical properties are summarized in Table 2.
Table 1. Chemical Composition of the Cold-Rolled and Annealed S31254 Stainless Steel Strip
Chemical composition (wt.%)
|
Element |
Mo |
Cr |
Ni |
Cu |
N |
C |
Mn |
Si |
P |
S |
|
Measured value |
6.2 |
20.2 |
17.9 |
0.74 |
0.21 |
0.011 |
0.28 |
0.43 |
0.023 |
0 |
|
Standard requirement |
6.0–6.5 |
19.5–20.5 |
17.5–18.5 |
0.5–1.0 |
0.18–0.25 |
≤0.02 |
≤1.0 |
≤0.8 |
≤0.03 |
≤0.01 |
Table 2. Mechanical Properties of the Cold-Rolled and Annealed S31254 Stainless Steel Strip
|
Item |
Tensile Strength, Rm (MPa) |
0.2% Proof Strength, Rp0.2 (MPa) |
Elongation, A5 (%) |
Hardness (HRB) |
|
Measured value |
785 |
407 |
40 |
90 |
|
Standard requirement |
≥690 |
≥310 |
≥35 |
≤96 |
The manufacturing process for straight-seam welded stainless steel pipes consists of the following steps:
Strip preparation → Cold roll forming → Welding → External weld bead grinding → Internal weld bead leveling → Primary sizing → In-line annealing → Secondary sizing → Eddy current testing → Laser diameter measurement → Cut-to-length processing → Chemical and mechanical testing → Ultrasonic testing → Underwater leak testing
Single-torch automatic tungsten inert gas (TIG) autogenous welding was employed to achieve single-sided welding with double-sided weld formation. During welding, 99.99% pure argon was supplied to the inside and outside of the pipe and through the welding torch to prevent high-temperature oxidation of the weld and base metal on both sides of the pipe. The welding speed was 0.9 m/min. The welding parameters used for the S31254 welded pipes are listed in Table 3.
Before welding, the strip edges were cleaned to remove contaminants such as oil, grease, and burrs. The vertical position and clamping force of the welding rolls were adjusted to maintain edge misalignment within 0.05 mm and the fit-up gap within 0.5 mm. Post-weld heat treatment was performed by in-line annealing at 1,180 °C. During annealing, both the inside and outside of the pipes were purged with 99.99% pure argon to prevent high-temperature oxidation of the weld and base metal.
Table 3. Welding Parameters for S31254 Welded Pipes
|
Welding speed (m/min) |
Welding current (A) |
Welding voltage (V) |
Torch angle (°) |
Torch shielding gas flow rate (L/min) |
Internal shielding gas flow rate (L/min) |
External shielding gas flow rate (L/min) |
|
0.9 |
116 |
10.9 |
75 |
16 |
18 |
40 |
Mechanical and process performance tests were conducted in accordance with ASTM A249/A249M. These included room-temperature tensile testing, hardness testing, reverse bend testing, flattening, flaring, and flanging. Weld cross-sections were examined to assess their macroscopic morphology and then polished and etched for metallographic examination. Intergranular corrosion testing was performed in accordance with Method E of ASTM A262, followed by a flattening test. Pitting corrosion resistance was evaluated in accordance with Method A of ASTM G48 by immersing the specimens in a 6% FeCl₃ solution at 50 °C for 72 h. Nondestructive testing (NDT) included eddy current testing, ultrasonic testing, and leak testing.
Room-temperature mechanical property tests were conducted on Φ32 mm × 1.2 mm welded pipes in accordance with ASTM A249/A249M-2024, Standard Specification for Welded Austenitic Steel Boiler, Superheater, Heat-Exchanger, and Condenser Tubes. Tensile and hardness specimens were prepared for testing. Tensile tests were performed on a universal testing machine (model CMT5105) using full-section pipe specimens loaded to fracture, as shown in Fig. 1. Hardness measurements were taken using a Brinell–Vickers hardness tester (model 402MVA).
The room-temperature mechanical properties of the S31254 welded pipes are presented in Table 4. The results show that the tensile strength, yield strength, and elongation all met the standard requirements. The weld zone exhibited the highest hardness, while the base metal had the lowest. The hardness values of the HAZ, weld zone, and base metal were all ≤100 HRB, with a maximum difference of ≤4.1 HRB.

(a) Specimen 1 (b) Specimen 2
Figure 1. Fractured S31254 welded pipe specimens after tensile testing
Table 4. Mechanical Properties of S31254 Welded Pipes
|
Parameter |
Tensile Strength (MPa) |
Yield Strength (MPa) |
Elongation (%) |
Weld Zone Hardness (HRB) |
Base Metal Hardness (HRB) |
HAZ Hardness (HRB) |
|
Specimen 1 |
807 |
469 |
45.8 |
93.7 |
91.9 |
93.4 |
|
Specimen 2 |
804 |
467 |
47.2 |
95.2 |
91.1 |
92.1 |
|
Standard requirements |
≥675 |
≥310 |
≥35 |
≤100 |
≤100 |
≤100 |
Process performance tests were conducted on the welded pipes in accordance with ASTM A249/A249M. Specimens were prepared for reverse bend, flattening, flaring, and flanging tests, which were performed using a universal testing machine or a compression testing machine. No visible cracks were observed on any of the specimen surfaces after testing. In particular, the flaring test was conducted using a mandrel angle of 60° and a flaring ratio of 24%. These results confirmed that the welded pipes passed all process performance tests.
A 10–15 mm-long cross-sectional specimen was cut from the welded pipe along its longitudinal axis using a laser cutting machine. The cross-section was then ground and polished, and its macroscopic features were examined using an XJZ-6A metallographic microscope equipped with an imaging system. The thickness difference between the weld/fusion line and the base metal was within 0.028 mm. The weld profile was smooth, with no visible defects such as cracks, incomplete penetration, incomplete fusion, or undercut. Weld reinforcement was well controlled, and the overall weld appearance was satisfactory. The macroscopic appearance of the S31254 welded pipe specimen is shown in Fig. 2, and the corresponding dimensional measurements are presented in Table 5.

(a) Weld (b) Base metal
Figure 2. Measurement locations in the weld and base metal of the S31254 welded pipe
Table 5 Weld Dimensions of S31254 Welded Pipe Specimens
|
Maximum weld thickness (mm) |
Fusion line 1 thickness (mm) |
Fusion line 2 thickness (mm) |
Base metal thickness (mm) |
Weld reinforcement (mm) |
|
1.252 |
1.239 |
1.256 |
1.224 |
0.028 |
Metallographic examination was performed on the Φ32 mm × 1.2 mm S31254 welded pipes. The specimens were polished and etched using a solution of HCl, HNO₃, and H₂O mixed in a volume ratio of 1:1:1. The microstructures were observed using an XJZ-6A metallographic microscope, and the results are presented in Fig. 3. As shown in Fig. 3, the base metal, weld zone, and heat-affected zone (HAZ) all exhibited an austenitic microstructure. The base metal contained some twins and precipitates, whereas the weld zone and HAZ were predominantly characterized by columnar dendritic austenite.

(a) Base metal (b) Weld zone (c) Fusion line 1 (d) Fusion line 2
Figure 3. Microstructures of the S31254 welded pipe
Intergranular corrosion testing was conducted in accordance with Method E of ASTM A262-15 (2021), Standard Practices for Detecting Susceptibility to Intergranular Attack in Austenitic Stainless Steels. The base metal, weld zone, and heat-affected zone (HAZ) were examined at ×40 magnification using a VMS300 video measuring system. No intergranular corrosion cracks were observed in any of the three regions. A flattening test was then performed. The specimens were compressed until the gap between their inner walls reached 5 mm and 2 mm, respectively, with the weld oriented at 90° to the direction of the applied force. No cracks were observed in either the base metal or the weld zone. Figure 4 shows the S31254 welded pipe specimens after corrosion exposure and subsequent flattening.
Pitting corrosion testing was conducted in accordance with Method A of ASTM G48-25, Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution. The test solution, containing approximately 6 wt.% FeCl₃, was prepared by dissolving 100 g of reagent-grade ferric chloride hexahydrate (FeCl₃·6H₂O) in 900 mL of Type IV reagent water. The specimens were immersed in the solution at 50 °C for 72 h. Examination at ×20 magnification revealed no pitting on the surfaces of the base metal, weld zone, or heat-affected zone (HAZ).

(a) Inner wall gap of 5 mm (b) Inner wall gap of 2 mm
Figure 4. S31254 welded pipe specimens after corrosion testing and subsequent flattening
Eddy current testing was performed on the S31254 welded pipes (Φ32 mm × 1.2 mm) in accordance with ASTM A249/A249M using an IDEA0102 testing system. The artificial defect diameter was ≤0.7 mm, and the probe-to-pipe fill factor (coupling ratio) was ≥0.8. Ultrasonic testing was conducted in accordance with ASTM E213. Before testing, the equipment was calibrated using a reference pipe containing an artificial U-shaped notch along the weld seam. The notch dimensions were ≤0.22 mm in width, 0.15 mm in depth, and 12.7 mm in length. Leak testing was performed in accordance with ASTM A1016/A1016M to verify the sealing integrity of the welded pipes. The test pressure was ≥1.0 MPa, and the holding time was ≥10 s. The results of all three tests met the applicable acceptance requirements, confirming that the S31254 welded pipes passed nondestructive inspection.
(1) S31254 super-austenitic stainless steel exhibits excellent weldability. Using an automated single-torch tungsten inert gas (TIG) autogenous welding process, the pipes were welded from one side with full penetration, producing welds on both the inner and outer surfaces. Subsequent leveling of the internal weld bead resulted in smooth, uniform weld seams on both sides, with seamless transitions to the base metal. The welds exhibited excellent surface quality, with no visible defects, consistent quality, and high welding efficiency.
(2) In-line annealing was performed at 1,180 °C under a protective atmosphere of 99.99% pure argon on both the inner and outer surfaces of the pipe. The base metal, weld zone, and heat-affected zone (HAZ) all exhibited an austenitic microstructure. The welded pipes demonstrated good corrosion resistance and overall performance, with their corrosion resistance and mechanical properties meeting the applicable standard requirements. The hardness values of the HAZ, weld zone, and base metal were all ≤100 HRB, with a maximum difference of ≤4.1 HRB.
(3) The small-diameter S31254 super-austenitic stainless steel welded pipes (Φ32 mm × 1.2 mm) manufactured using this process successfully passed eddy current testing, ultrasonic testing, and pneumatic leak testing in accordance with the applicable ASTM standards. The process is suitable for batch production and provides a technical reference for the manufacture of other types of super-austenitic stainless steel welded pipes.