Welcome to China B2B Marketplace
Back to Supplier News
XIAMEN LANDEE INDUSTRIES CO., LTD.

Synthesis Gas Waste Heat Boiler Tube-to-Tubesheet Joint Leakage: Causes and Corrective Measures

Nov 24, 2026
0 views
Synthesis Gas Waste Heat Boiler Tube-to-Tubesheet Joint Leakage: Causes and Corrective Measures
On this page

Abstract: This study investigates recurring leakage at the tube-to-tubesheet joints of a synthesis gas waste heat boiler in a large-scale ammonia synthesis plant. The boiler operates under demanding conditions involving high temperature, high pressure, a hydrogen-rich environment, and frequent start-stop cycles. A systematic failure analysis was conducted, covering:

  • Macroscopic examination and nondestructive testing
  • Verification of the design specifications and welding procedures
  • Evaluation of the materials and operating conditions.

 

The investigation identified the distribution patterns of cracks at the joints and examined their development. The results indicate that the absence of postweld heat treatment (PWHT) allowed welding residual stresses to combine with thermal stresses arising from the mismatch in thermal expansion between the 15CrMo tubes and the 304 stainless steel weld overlay. This interaction resulted in localized stress concentrations. Under repeated thermal cycling and exposure to a high-temperature, hydrogen-rich environment, cracks initiated at the joints and progressively propagated, eventually causing leakage.

Based on established design practices for similar heat exchangers operating under high-temperature hydrogen service, this study proposes structural and process improvements focusing on three areas:

  • Improving material compatibility
  • Optimizing welding procedures
  • Enhancing residual stress control.

 

In modern process industries, including ammonia synthesis, hydrogen production, and methanol synthesis, synthesis gas waste heat boilers play a vital role in recovering process waste heat and maintaining the overall energy balance. Their operational stability directly affects plant energy efficiency and economic performance. Operating for extended periods under demanding conditions, these boilers are exposed to the following conditions:

  • High temperatures, often exceeding 400°C
  • High operating pressures
  • Hydrogen-rich environments
  • Complex gas compositions containing various impurities.

These conditions make synthesis gas waste heat boilers particularly susceptible to operational failures. As a critical part of the pressure-retaining boundary, the tube-to-tubesheet joints are especially vulnerable to leakage, which can have serious consequences for equipment integrity and plant operation.

Leakage at these joints generally results from the combined effects of several damage mechanisms, including:

  • Stress corrosion cracking
  • High-temperature hydrogen attack
  • Thermal fatigue
  • Vibration-induced wear

 

Although the macroscopic failure modes of such equipment have been widely studied, the investigation of specific engineering failures requires a comprehensive analysis that considers equipment operating history, process conditions, material selection, and microscopic damage characteristics. Such an approach is essential for identifying the root causes of failure and developing effective improvement measures.

 

This paper presents a systematic failure analysis of recurring leakage at the tube joints of a synthesis gas waste heat boiler in a 500,000 t/a ammonia synthesis plant. The investigation adopts a comprehensive approach involving:

  • Macroscopic examination
  • Nondestructive testing (NDT)
  • Design review
  • Analysis of materials and process media
  • Comparison with the designs of similar equipment

The aim is to identify the primary failure mechanisms and contributing factors under the actual operating conditions. The findings provide a basis for targeted design optimization and process improvements, as well as practical guidance for the preventive maintenance, risk management, and service life assessment of similar equipment.

 

1 Equipment Specifications and Configuration

The synthesis gas waste heat boiler is a U-tube heat exchanger with a clamped tubesheet design, as shown in Figure 1. Its main design parameters are as follows:

(1) Tube side: The process medium is methane-rich synthesis gas. The design pressure is 2.84 MPa, compared with an operating pressure of 2.58 MPa. The design temperature is 450°C, and the operating temperature ranges from 335 to 445°C.

(2) Shell side: The medium consists of boiler feedwater and steam. The design pressure is 3.46 MPa, compared with an operating pressure of 3.3 MPa. The design temperature is 245°C, and the operating temperature is approximately 240°C.

(3) Main materials: The channel is made of 15CrMoR, the shell is made of Q345R, the tubes are made of 15CrMo, and the tubesheet consists of a 15CrMo III base material with an SS304 weld overlay.

Notably, the joints between the 15CrMo tubes and the SS304 weld overlay on the tubesheet are dissimilar-metal welded joints. Postweld stress-relief heat treatment for these joints was not specified in the design or performed during manufacturing.

 

2 Incident Overview and Inspection Findings

Since commissioning, the synthesis gas waste heat boiler has operated primarily at approximately 60% of its rated load, with frequent start-stop cycles. During operation, recurring leakage occurred at the welded joints between the tubes and the tubesheet. Initially, the leaking tubes were plugged. However, the number of leaking tubes continued to increase, with no discernible pattern in their distribution across the tubesheet. Following replacement of the entire tube bundle, the boiler operated for only about one year before leakage recurred in more than a dozen tubes.

 

On-site inspection revealed that leakage was concentrated in two areas: the fillet welds connecting the tubes to the tubesheet and the protruding tube ends beyond the tubesheet. Penetrant testing (PT) revealed circumferential cracks in most of the fillet welds, whereas extensive longitudinal cracks were found at the protruding tube ends. Some of these cracks had developed into clearly visible open fractures. Further examination of the channel and other areas of the tubesheet revealed no significant evidence of general corrosion or cracking. Figure 2 shows typical crack locations, while Figure 3 illustrates the distribution of leaking tubes across the tubesheet.

 

Figure 1. Structure of the Synthesis Gas Waste Heat Boiler

 

Figure 2. Typical Crack Locations

 

Figure 3. Distribution of Leaking Tubes Across the Tubesheet

 

 

3 Failure Analysis

3.1 Process Medium and Operating Environment

According to the equipment data sheet, the tube-side medium is hydrogen-rich synthesis gas containing no H₂S, with an inlet temperature of up to 445°C. Its typical outlet composition is listed in Table 1, indicating a typical high-temperature hydrogen service environment. Although no characteristic signs of high-temperature hydrogen attack (HTHA), such as decarburization or microcracking, were observed during the inspection, prolonged exposure to this environment may increase the material's susceptibility to hydrogen-related damage. In addition, frequent startup and shutdown cycles cause repeated temperature fluctuations, creating favorable conditions for thermal fatigue crack initiation. During shutdown, if the temperature drops below the dew point, CO₂ and water vapor in the process gas may condense and form carbonic acid, potentially initiating corrosion and aggravating localized damage.

 

3.2 Welding Procedure Review

A review of the welding documentation and on-site inspection of the welded joints confirmed that the tubesheet has a 304 austenitic stainless steel weld overlay. The tube-to-tubesheet joints were welded by shielded metal arc welding (SMAW) using 3.2 mm diameter ENiCrFe-3 nickel-based electrodes.

 

3.3 Comparison with Similar Equipment Designs

For tube-to-tubesheet joints connecting Cr-Mo steel tubes to tubesheets in high-temperature, hydrogen-rich service, internationally recognized licensors, including Casale, Topsøe, and KBR, typically recommend two design approaches:

Table 1. Composition of the Tube-Side Outlet Gas in the Synthesis Gas Waste Heat Boiler

Component

CH₄

NH₃

H₂

N₂

CO

CO₂

Ar

H₂O

Flow rate (kmol/h)

8.13

0.56

1,182.79

76.54

276.04

238.65

1.83

1,424.84

Mole fraction (mol%)

0.25

0.02

36.85

2.38

8.60

7.44

0.06

44.40

 

(1) Welding with Matching Materials: The tubesheet is made of Cr-Mo steel without a weld overlay and is welded directly to the Cr-Mo steel tubes. Gas tungsten arc welding (GTAW) is recommended because it allows more precise control of heat input.

(2) Welding to a Dissimilar-Metal Weld Overlay: The tubesheet consists of a Cr-Mo steel base material with a weld overlay at least 6 mm thick, deposited in two layers using Alloy 625 (e.g., Inconel 625). The tubes are then welded to the overlay by GTAW. The Cr-Mo steel tubesheet with the weld overlay is shown in Figure 4.

 

Figure 4. Cr-Mo Steel Tubesheet with Alloy 625 Weld Overlay

 

Both options require postweld heat treatment (PWHT) to relieve residual stresses. A key advantage of Option 2 is that, if leakage occurs during operation, on-site repair welding can be carried out using ERNiCrMo-3 filler metal without requiring complex on-site heat treatment. This significantly simplifies repair work.

 

4 Leakage and Failure Mechanisms of Tube-to-Tubesheet Joints in Heat Exchangers

Based on the above investigation, leakage at the tube-to-tubesheet joints resulted from the combined effects of multiple factors. The main contributing factors are summarized as follows:

(1) High welding residual stress: The original design specified shielded metal arc welding (SMAW), a process with relatively high heat input that is difficult to control precisely. This resulted in substantial residual stresses in the weld seams and heat-affected zones (HAZs). Furthermore, postweld heat treatment (PWHT) of the tube-to-tubesheet joints was not included in the design or manufacturing process, leaving high residual stresses in the joints and contributing to localized stress concentrations.

 

(2) Thermal stress caused by material mismatch: The linear thermal expansion coefficients of 15CrMo and 304 stainless steel (304SS) differ significantly. Their average values over the operating temperature range are approximately 1.3 × 10⁻⁵/°C and 1.92 × 10⁻⁵/°C, respectively. As the equipment heats up from ambient temperature to above 400°C, the two materials undergo different amounts of thermal expansion, generating additional thermal stresses at the joints. These stresses combine with the welding residual stresses, increasing the risk of tube-to-tubesheet joint failure.

 

(3) Environmental and operational contributing factors

① Thermal fatigue: Frequent startup and shutdown cycles subject the joints to repeated thermal fluctuations, promoting fatigue crack initiation and propagation in regions of high stress concentration.

② Environmental effects: Although no significant macroscopic evidence of hydrogen-induced damage was observed, prolonged exposure to a high-temperature, hydrogen-rich environment may have promoted hydrogen adsorption and diffusion in highly stressed regions, potentially accelerating crack propagation. In addition, condensation of water vapor during shutdown, in the presence of CO₂, may have resulted in carbonic acid formation and created a corrosive environment at crack tips, further aggravating localized damage.

③ Failure mechanism: The overall failure process can be summarized as follows:

Inadequate welding procedures and the absence of postweld heat treatment → High welding residual stresses combined with thermal stresses caused by material mismatch → Localized stress concentrations at the joints → Repeated thermal cycling and exposure to a potentially corrosive environment → Crack initiation and propagation → Process medium leakage.

 

5 Structural and Process Improvements

To address the failure mechanisms identified above, the improvement measures should focus on reducing stress levels in the joint regions and improving the structure's ability to withstand demanding operating conditions. This requires a systematic approach to optimizing the design, material selection, welding procedures, and residual stress control.

 

5.1 Optimization of Tubesheet Material Selection and Structural Design

Recommended approach: To minimize thermal stresses caused by differences in thermal expansion, priority should be given to material combinations with closely matched coefficients of thermal expansion (CTEs).

Option 1: Direct Welding Using Matching Materials. The tubesheet is made of 15CrMo IV forgings and is welded directly to the 15CrMo tubes. This material combination results in a similar-metal welded joint, avoiding the material incompatibility associated with dissimilar-metal welding.

Option 2: Welding to an Inconel 625 Weld Overlay. The tubesheet is made of 15CrMo IV forgings with an Inconel 625 alloy weld overlay at least 6 mm thick. The tubes are then welded directly to the overlay. The average linear coefficient of thermal expansion of Inconel 625 over the equipment's operating temperature range is approximately 1.33 × 10⁻⁵/°C, which is close to that of 15CrMo. This helps reduce thermal stresses caused by the mismatch in thermal expansion. Option 2 offers practical advantages in engineering applications because it maintains joint performance while facilitating subsequent on-site repair welding without the need for PWHT.

 

5.2 Improvements to Welding Procedures and Quality Control

Welding method: Replace shielded metal arc welding (SMAW) with gas tungsten arc welding (GTAW) for the tube-to-tubesheet joints. GTAW provides a concentrated heat source and allows more precise control of heat input. It also produces a high-quality weld profile and generally results in lower residual stresses.

Welding consumables: When Option 2 is adopted, ERNiCrMo-3 filler wire conforming to AWS A5.14 is recommended for welding the tubes to the Inconel 625 overlay. This filler metal provides good metallurgical compatibility with the overlay and suitable high-temperature properties.

Process control: Develop and strictly implement a detailed Welding Procedure Specification (WPS). Key parameters, including shielding gas purity, welding current, voltage, travel speed, and interpass temperature, should be rigorously controlled to ensure consistent weld quality and full process traceability.

 

5.3 Mandatory Postweld Heat Treatment (PWHT)

Regardless of the improvement option selected, the welded tube-to-tubesheet joints must undergo stress-relief heat treatment promptly after welding. The heat treatment procedure must be developed and implemented in strict accordance with the applicable standards, including GB/T 150-2024, GB/T 30583-2026, and NB/T 47015-2023. This treatment is intended to reduce and homogenize welding residual stresses, thereby improving the joints' resistance to stress corrosion cracking and fatigue.

 

5.4 Operational and Maintenance Recommendations

Optimize startup and shutdown procedures to minimize rapid temperature fluctuations and frequent load changes, thereby reducing thermal fatigue. During shutdowns, strictly follow the prescribed procedure for rapidly purging process gases with nitrogen to prevent condensate from forming inside the tubes and avoid dew-point corrosion. Give tube-joint areas priority during routine inspections. During major overhauls, perform liquid penetrant testing or more advanced non-destructive testing (NDT) to detect and address potential defects at an early stage.

 

6 Conclusion

The analysis indicates that recurring leakage at the tube-to-tubesheet joints of the syngas waste heat boiler results not from a single cause but from the combined effects of welding residual stress, thermal mismatch stress between dissimilar materials, operating conditions, and the process environment. In particular, the superposition of stresses under high-temperature conditions is the primary driver of crack initiation and propagation in the joint regions. For critical equipment operating under severe service conditions, particularly in high-temperature, hydrogen-rich environments, material compatibility, manufacturing process integrity, and residual stress control must be rigorously addressed during the design phase. These measures improve equipment safety at the source and help ensure long-term, reliable operation.

Comments

Leave a Comment

Related Supplier News